What causes coating delamination in tungsten carbide coatings prepared via HVOF spraying?
Industry News

What causes coating delamination in tungsten carbide coatings prepared via HVOF spraying?

2026-10-14

Hello everyone, this is Chengdu Daguang, a manufacturer that has been producing thermal spray powders since 1996. In this episode, we will focus on how to prevent the peeling or delamination of tungsten carbide coatings applied via the HVOF (High-Velocity Oxy-Fuel) process.

First, let’s look at a few photos showing coating delamination—specifically, examples of typical peeling occurring either immediately after spraying or during actual service.

14.png 15.png

Setting aside improper spraying techniques, the primary reasons for the delamination of HVOF-sprayed tungsten carbide coatings include the following:

1: The operating conditions are unsuitable for the HVOF spraying process.

2: Improper substrate preparation.

3: Excessive operating temperatures.

4: Premature failure of the sealer.

5: Use of excessively coarse powder.

6: The coating is too thick.

Point 1: The operating conditions are unsuitable for coatings produced via supersonic spraying.

Coatings produced by supersonic spraying exhibit a bond strength of approximately 50–100 MPa, which is essentially a mechanical bond. Compared to processes such as oxy-acetylene spray-welding, plasma surfacing, and laser cladding, supersonic spraying offers relatively low bond strength. Consequently, if the operating environment involves impacts from hard objects, the coating is liable to chip or peel off.

For instance, harvester blades frequently encounter stones during operation; therefore, tungsten carbide coatings applied via supersonic spraying are unsuitable for them—processes offering higher bond strength, such as laser cladding, are preferable. In contrast, industrial paper-cutting blades are well-suited for tungsten carbide coatings applied via supersonic spraying.

16.png 17.jpg

Point 2: Improper substrate preparation

This issue encompasses several scenarios. For instance, if the substrate is not thoroughly cleaned of rust or oil, the bond strength of the subsequent coating will be compromised. Another commonly overlooked issue arises when the substrate is harder than ordinary steel—such as chilled cast iron. Standard sandblasting fails to achieve sufficient surface roughness on such hard materials; instead, one should switch to a harder abrasive (like white fused alumina) with a coarser grit size and increase the blasting pressure.

Point 3: Excessive operating temperature

A primary cause here is the significant disparity between the thermal expansion coefficients of typical steels and tungsten carbide; this mismatch can lead to coating delamination. To prevent this, a NiCr (Ni80Cr20) transition layer should be applied prior to the tungsten carbide coating to alleviate interfacial stress caused by the difference in thermal expansion. Additionally, when operating temperatures exceed 500°C, tungsten carbide undergoes significant oxidation and decarburization (WC → W₂C); in such cases, a more heat-resistant material, such as nickel-chromium-chromium carbide (NiCr-Cr₃C₂), should be used instead.

Point 4: Premature failure of the sealer

This issue typically arises in corrosive environments. Tungsten carbide coatings produced via HVOF (High-Velocity Oxy-Fuel) spraying usually possess a residual porosity of less than 1%. When the operating environment is corrosive, a sealer is applied to fill these remaining pores and prevent corrosive agents from penetrating to the substrate and causing corrosion. A common failure scenario involves the substrate rusting prematurely; as rust accumulates between the coating and the substrate, the bond strength is drastically reduced, ultimately leading to coating delamination.

18.png

Point 5: Using too coarse powder

Supersonic spraying conventionally uses 5-45 micron powder. If coarser powder is used to achieve greater roughness, it will lead to poor bonding strength of the coating and premature shedding during later use.

Point 6: The coating is too thick. The coating of supersonic spraying should usually not exceed 50 wires. The thickness of 2-5 wires can be applied in each pass. As mentioned earlier, supersonic spraying is a mechanical combination, so it cannot be a few millimeters thick like laser cladding and plasma cladding. If it is too thick, the bonding strength will also be reduced.